Piezo Ceramics Description:
R45mm
Material:PZT-82
Frequency:3Mhz
Performance Parameter:
Fs(Hz):89936
Fp(Hz):104720
Kp:0.578
ft(MHZ):2.997
C(pf): 7550
Application of HIFU Piezo Ceramic:
Ultrasonic focus ceramic (HIFU) is widely used in the beauty, weight loss medical industry and liposonix,ultra Shape.On behalf of the product is this year the rise of the ultrasonic knife, Liposonix slimming Instrument,Ultra Shape slimming instrument.
High Intensity Focused Ultrasound(HIFU):
High Intensity Focused Ultrasound is a non-surgical, no downtime, in-office procedure for lifting and tightening sagging skin of the brows, cheeks, lower face (jowls), jawline and neck. Ultrasound technology is focused below the skin surface to firm and lift droopy tissues. Results are long lasting and occur gradually but dramatically over time.
Standard Size of HIFU Piezo Ceramic:
Working Frequency : 1 ~ 10 MHz (Selectable)
Aperture size : Diameter 20 ~ 70mm(Selectable)
Focal length: 10 ~ 100 mm (Selelctable)
Strong Electrode: Silvering ,Nickel, Titanium Alloys
Long Lifetime: high power pulses>15000
Typical value of "Hard" PZT materials performance:
Hard" PZT materials |
PZT-41 |
PZT-42 |
PZT-43/4D |
PZT-82 |
PBaS-4 |
||
Dielectric Constant |
ɛTr3 |
1050 |
1250 |
1420 |
1100 |
1900 |
|
Coupling factor |
KP |
0.58 |
0.58 |
0.58 |
0.52 |
0.59 |
|
K31 |
0.32 |
0.33 |
0.34 |
0.3 |
0.34 |
||
K33 |
0.66 |
0.67 |
0.68 |
0.57 |
0.68 |
||
Kt |
0.48 |
0.48 |
0.48 |
0.4 |
0.49 |
||
Piezoelectric coefficient |
d31 |
10-12m/v |
-106 |
-124 |
-138 |
-100 |
-160 |
d33 |
10-12m/v |
260 |
280 |
300 |
240 |
380 |
|
g31 |
10-3vm/n |
-11.4 |
-11.2 |
-11 |
-10.3 |
-9.5 |
|
g33 |
10-3vm/n |
28 |
25.3 |
24 |
25 |
22.6 |
|
Frequency coefficients |
Np |
2280 |
2200 |
2160 |
2280 |
2200 |
|
N1 |
1671 |
1613 |
1583 |
1671 |
1613 |
||
N3 |
1950 |
1900 |
1875 |
1950 |
1850 |
||
Nt |
2250 |
2200 |
2200 |
2300 |
2200 |
||
Elastic compliance coefficient |
Se11 |
10-12m2/n |
11.8 |
12.7 |
13.2 |
11.6 |
13.2 |
Machanical quality factor |
Qm |
1000 |
800 |
600 |
1200 |
2200 |
|
Dielectric loss factor |
Tg δ |
% |
0.3 |
0.4 |
0.5 |
0.3 |
0.5 |
Density |
ρ |
g/cm3 |
7.5 |
7.5 |
7.5 |
7.6 |
7.5 |
Curie Temperature |
Tc |
°C |
320 |
320 |
320 |
310 |
310 |
Young's modulus |
YE11 |
<109N/m3 |
85 |
79 |
76 |
86 |
76 |
Poison Ratio |
0.3 |
0.3 |
0.3 |
0.3 |
0.33 |